spacer


Title - Auger Parameter Energies

        
Navigation Bar Navigation Bar


bar

 

Ce, Cerium

bar

CERIUM S E 3d5/2 4d5/2 Ref.
Ce 3 1 (883.9)   82-27
CeAl2     883.5 109.1 80-17
CePd3     884.3   80-17
CeH2     885.8   82-27
CeH3 2   886.0   82- 27
CeSe     884.3   80- 17
CeCu2Si2     883.6   80-17
Ce2(MoO4)3     881.7   83- 3
CeO2 4 1 881.93   83- 3
 

bar

 
Notes
S Number of independent studies (where this is greater than 1)
E Number of these rejected as unsound (mainly early measurements) before the remaining ones were used to determine a mean value
A.P Auger parameter (calculated from the most intense photoelectron line and Auger line)
M.A.P. Modified Auger Parameter
v Referenced to the vacuum level (gases)
c Includes minor corrections in high binding energy lines using X-ray energy data from reference 67-1
Refs. Reference in which the data was originally published. (See the references section)
  

bar

bar

Navigation Bar Navigation Bar

bar

Last updated 24 February, 2001

Compiled by and
Christopher Walker
KLA-Tencor,
686 Stirling Road
Slough
Berks., UK
Simon Morton
Advanced Light Source
Lawrence Berkeley Laboratory
Berkeley
CA 94720
email chris.walker@physics.org email S.Morton@uksaf.org

bar
© UK Surface Analysis Forum 1998