MOLYBDENUM S E 3d5/2 M5VV A.P. Ref.
Mo     227.85     81-22
Mo 13 3 227.9 222.8 450.7 79-18
Mo     228.0 2038.8t 2266.8t 80-35
MoB2     227.9     73-11
Mo2C     227.8     78-2
MoSi2 2   227.68 2039.0t 2266.7t 82-23
MoSe2     228.3     75-8
MoS2 8 2 229.0     80-38
MoO2 12 4 229.6     82-5
MoO3 17 2 232.8     82-5
Al2(MoO4)3 3   232.7     80-38
CoMoO4 5 3 233.1     76-13
K2MoO4     232.1     82-12
CoMo2S4     228.7     82-1
InMo6S8     227.9     85-9
Na2MoO4 4   232.0     82-12
Rh2MoO6     231.8     82-12
MoOCl3(PPh3)2     232.3     74-7
MoCl3     230.6     80-26
MoCl4     230.6     75- 8
MoCl5 2   231.0     75-8
 

bar

 

t Lines L3M45M45 and corresponding Auger parameter

 

bar

 
Notes
S Number of independent studies (where this is greater than 1)
E Number of these rejected as unsound (mainly early measurements) before the remaining ones were used to determine a mean value
A.P Auger parameter (calculated from the most intense photoelectron line and Auger line)
M.A.P. Modified Auger Parameter
v Referenced to the vacuum level (gases)
c Includes minor corrections in high binding energy lines using X-ray energy data from reference 67-1
Refs. Reference in which the data was originally published. (See the references section)
  

bar

bar

Navigation Bar Navigation Bar

bar

Last updated 24 February, 2001

Compiled by and
Christopher Walker
KLA-Tencor,
686 Stirling Road
Slough
Berks., UK
Simon Morton
Advanced Light Source
Lawrence Berkeley Laboratory
Berkeley
CA 94720
email chris.walker@physics.org email S.Morton@uksaf.org

bar
© UK Surface Analysis Forum 1998