NIOBIUM S E 2p3/2 Ref.
Nb 10 2 202.18 81-22
NbN     203.8 75-2
NbTe4     203.8 75-2
NbSe4     203.4 75-2
NbO 4 2 203.7 75-2
NbO2 5 2 205.7 75-2
Nb2O5 12 4 207.6 82-13
NbI5     207.1 84-6
NbBr5     207.1 73-12
NbCl5     208.0 73-12
RhNbO4     206.5 82-12
KNbO3     2a6.5 73-11
Ca2Nb2O7     206.7 75-2
K2NbF7     209.4 73-12
 

bar

 
Notes
S Number of independent studies (where this is greater than 1)
E Number of these rejected as unsound (mainly early measurements) before the remaining ones were used to determine a mean value
A.P Auger parameter (calculated from the most intense photoelectron line and Auger line)
M.A.P. Modified Auger Parameter
v Referenced to the vacuum level (gases)
c Includes minor corrections in high binding energy lines using X-ray energy data from reference 67-1
Refs. Reference in which the data was originally published. (See the references section)
  

bar

bar

Navigation Bar Navigation Bar

bar

Last updated 24 February, 2001

Compiled by and
Christopher Walker
KLA-Tencor,
686 Stirling Road
Slough
Berks., UK
Simon Morton
Advanced Light Source
Lawrence Berkeley Laboratory
Berkeley
CA 94720
email chris.walker@physics.org email S.Morton@uksaf.org

bar
© UK Surface Analysis Forum 1998