| OXYGEN |
S |
E |
1s |
Ref. |
| CdO |
4 |
|
529.2 |
82-12 |
| CeO2 |
4 |
|
529.2 |
75-11 |
| RuO2 |
4 |
|
529.4 |
80-28 |
| SnO2 |
4 |
|
530.6 |
78-6 |
| NiO |
10 |
|
529.5 |
84-10 |
| Ni(OH)2 |
9 |
|
531.2 |
84- 10 |
| CuO |
9 |
1 |
529.6 |
81 11 |
| Cu2O |
7 |
1 |
530.4 |
81 11 |
| CoO |
7 |
|
530.2 |
75 11 |
| Co~O4 |
6 |
|
53().2 |
75-11 |
| Fe3O4 |
4 |
|
530.() |
80-7 |
| Na2MoO4 |
3 |
|
530.2 |
77-17 |
| MoO3 |
11 |
2 |
530.62 |
83-3 |
| Al2O3 |
17 |
4 |
531.0 |
84-21 |
| CaCO ~ |
3 |
|
531.4 |
83-5 |
| BeO |
4 |
|
531.6 |
82-12 |
| KC103-3 |
|
|
531.87 |
85-13 |
| KCI04-3 |
|
|
532.92 |
85-13 |
| poly(CH2( HOH) |
3 |
|
532.6 |
77-20 |
| H 2O |
3 |
1 |
533. I |
80-34 |
| Co(CO)6 |
5 |
1 |
533.9 |
76-10 |
|
| |

|
| |
Notes
| S |
Number of independent studies (where this is greater than 1) |
| E |
Number of these rejected as unsound (mainly early measurements) before the remaining
ones were used to determine a mean value |
| A.P |
Auger parameter (calculated from the most intense photoelectron line and Auger line) |
| M.A.P. |
Modified Auger Parameter |
| v |
Referenced to the vacuum level (gases) |
| c |
Includes minor corrections in high binding energy lines using X-ray energy data from reference 67-1 |
| Refs. |
Reference in which the data was originally published. (See the references
section) |
|
| |

|


Last updated 24 February, 2001
| Compiled by |
and |
Christopher Walker
KLA-Tencor,
686 Stirling Road
Slough
Berks., UK |
Simon Morton
Advanced Light Source
Lawrence Berkeley Laboratory
Berkeley
CA 94720 |
| email chris.walker@physics.org |
email S.Morton@uksaf.org |

© UK Surface Analysis Forum 1998
|
|